Acta Metallurgica Sinica (English Letters) ›› 2019, Vol. 32 ›› Issue (3): 372-380.DOI: 10.1007/s40195-018-0786-5
Special Issue: 2018-2019高温合金专辑
• Orginal Article • Previous Articles Next Articles
					
													An-Wen Zhang1,2, Yang Li1, Sha Zhang1, Fang Liu1, Wei-Hong Zhang1, Lian-Xu Yu1, Wen-Ru Sun1(
)
												  
						
						
						
					
				
Received:2018-04-25
															
							
																	Revised:2018-06-26
															
							
															
							
																	Online:2019-03-10
															
							
																	Published:2019-02-22
															
						An-Wen Zhang, Yang Li, Sha Zhang, Fang Liu, Wei-Hong Zhang, Lian-Xu Yu, Wen-Ru Sun. Re-recognition of the Effects of Phosphorus and Boron on the γ″ and γ′ Phases in IN718 Alloy[J]. Acta Metallurgica Sinica (English Letters), 2019, 32(3): 372-380.
Add to citation manager EndNote|Ris|BibTeX
| Master alloy no. | Ni | Fe | Cr | Al | Ti | Nb | Mo | C | 
|---|---|---|---|---|---|---|---|---|
| A | 52.7 | Bal. | 19.18 | 0.64 | 1.11 | 5.22 | 3.05 | 0.058 | 
| B | 52.6 | Bal. | 19.12 | 0.50 | 0.86 | 4.99 | 3.01 | 0.46 | 
| C | 52.3 | Bal. | 19.15 | 0.48 | 0.90 | 5.30 | 3.08 | 0.043 | 
Table 1 Analyzed concentrations of the three master ingots (mass%)
| Master alloy no. | Ni | Fe | Cr | Al | Ti | Nb | Mo | C | 
|---|---|---|---|---|---|---|---|---|
| A | 52.7 | Bal. | 19.18 | 0.64 | 1.11 | 5.22 | 3.05 | 0.058 | 
| B | 52.6 | Bal. | 19.12 | 0.50 | 0.86 | 4.99 | 3.01 | 0.46 | 
| C | 52.3 | Bal. | 19.15 | 0.48 | 0.90 | 5.30 | 3.08 | 0.043 | 
| Alloy no. | P (mass%) | P (atomic%) | B (mass%) | B (atomic%) | 
|---|---|---|---|---|
| A1 | 0.001 | 0.002 | 0.0046 | 0.024 | 
| A2 | 0.017 | 0.031 | 0.009 | 0.048 | 
| B1 | 0.001 | 0.002 | 0.004 | 0.022 | 
| B2 | 0.001 | 0.002 | 0.010 | 0.054 | 
| C1 | 0.001 | 0.002 | 0.005 | 0.026 | 
| C2 | 0.015 | 0.028 | 0.005 | 0.026 | 
Table 2 Analyzed compositions of the six alloys
| Alloy no. | P (mass%) | P (atomic%) | B (mass%) | B (atomic%) | 
|---|---|---|---|---|
| A1 | 0.001 | 0.002 | 0.0046 | 0.024 | 
| A2 | 0.017 | 0.031 | 0.009 | 0.048 | 
| B1 | 0.001 | 0.002 | 0.004 | 0.022 | 
| B2 | 0.001 | 0.002 | 0.010 | 0.054 | 
| C1 | 0.001 | 0.002 | 0.005 | 0.026 | 
| C2 | 0.015 | 0.028 | 0.005 | 0.026 | 
																													Fig. 4 Alloys A1 and A2 cooled by WQ after homogenization, dark-field images of γ″ and γ′ phases and the SAED patterns with [001] zone axis: a Alloy A1, viewed along a (0 1 0) direction; b Alloy A1, viewed along a (1 1/1221/122 0) direction.; c Alloy A2, viewed along a (0 1 0) direction; d Alloy A2, viewed along a (1 1/1221/122 0) direction
																													Fig. 5 Alloys A1 and A2 cooled by AC after homogenization, dark-field image of γ″ and γ′ phases and the SAED patterns with [001] zone axis: a Alloy A1, viewed along a (0 1 0) direction; b Alloy A1, viewed along a (1 1/1221/122 0) direction.; c Alloy A2, viewed along a (0 1 0) direction; d Alloy A2, viewed along a (1 1/1221/122 0) direction
| Phase | Supercell | ?fH (eV/atom) | 
|---|---|---|
| Ni3Al (γ′) | Ni24Al8 | - 0.475 | 
| Ni24Al7-P | - 0.461 | |
| Ni23Al8-P | - 0.508 | |
| Ni3Nb (γ″) | Ni24Nb8 | - 0.329 | 
| Ni24Nb7-P | - 0.314 | |
| Ni23Nb8-P (Ni-1) | - 0.339 | |
| Ni23Nb8-P (Ni-2) | - 0.308 | 
Table 3 Effect of P on the formation enthalpies of γ″ and γ′ phases calculated by first-principle calculations
| Phase | Supercell | ?fH (eV/atom) | 
|---|---|---|
| Ni3Al (γ′) | Ni24Al8 | - 0.475 | 
| Ni24Al7-P | - 0.461 | |
| Ni23Al8-P | - 0.508 | |
| Ni3Nb (γ″) | Ni24Nb8 | - 0.329 | 
| Ni24Nb7-P | - 0.314 | |
| Ni23Nb8-P (Ni-1) | - 0.339 | |
| Ni23Nb8-P (Ni-2) | - 0.308 | 
 
  | 
									
| [1] | Tianbo Zhao, Yutaka S. Sato, Hiroyuki Kokawa, Kazuhiro Ito. Predicting Tensile Properties of Friction-Stir-Welded 6063 Aluminum with Experimentally Measured Welding Heat Input [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1235-1242. | 
| [2] | Yuan Yu, Peiying Shi, Kai Feng, Jiongjie Liu, Jun Cheng, Zhuhui Qiao, Jun Yang, Jinshan Li, Weimin Liu. Effects of Ti and Cu on the Microstructure Evolution of AlCoCrFeNi High-Entropy Alloy During Heat Treatment [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1077-1090. | 
| [3] | Yunhai Su, Xuewei Liang, Yunqi Liu, Zhiyong Dai. Effect of Ti Addition on the Microstructure and Property of FeAlCuCrNiMo0.6 High-Entropy Alloy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(7): 957-967. | 
| [4] | Yue Su, Shun-Cun Luo, Liang Meng, Piao Gao, Ze-Min Wang. Selective Laser Melting of In Situ TiB/Ti6Al4V Composites: Formability, Microstructure Evolution and Mechanical Performance [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(6): 774-788. | 
| [5] | Jin Hyuk Choi, Gobinda Gyawali, Dhani Ram Dhakal, Bhupendra Joshi, Soo Wohn Lee. Electrodeposited Ni-W-TiC Composite Coatings: Effect of TiC Reinforcement on Microstructural and Tribological Properties [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(4): 573-582. | 
| [6] | Sami Bin Humam, Gobinda Gyawali, Dhani Ram Dhakal, Jin-Hyuk Choi, Soo Wohn Lee. Effect of Pulse and Direct Current Electrodeposition on Microstructure, Surface, and Scratch Resistance Properties of Ni-W Alloy and Ni-W-SiC Composite Coatings [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(10): 1321-1330. | 
| [7] | Xiang-Qian Liu, Hui-Jie Liu, Yan Yu. Relationship Between Microstructures and Microhardness in High-Speed Friction Stir Welding of AA6005A-T6 Aluminum Hollow Extrusions [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(1): 115-126. | 
| [8] | Shuang-Jian Chen, Xiang-Xi Ye, D.K. L.Tsang, Li Jiang, Chao-Wen Li, Kun Yu, Zhi-Jun Li . Microstructure and Its Influence on the Mechanical Properties of Ni-28W-6Cr-Based Alloy-Welded Joints by GTAW [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(8): 1032-1040. | 
| [9] | N. Thangapandian, S. Balasivanandha Prabu , K. A. Padmanabhan. Effect of Temperature on Grain Size in AA6063 Aluminum Alloy Subjected to Repetitive Corrugation and Straightening [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(7): 835-844. | 
| [10] | Barros André, Cruz Clarissa, P. Silva Adrina, Cheung Noé, Garcia Amauri, Rocha Otávio, Moreira Antonio. Horizontally Solidified Al-3 wt%Cu-(0.5 wt%Mg) Alloys: Tailoring Thermal Parameters, Microstructure, Microhardness, and Corrosion Behavior [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(6): 695-709. | 
| [11] | Ge Bian, Ming Cheng, Yang Liu, Shi-Hong Zhang. Wear Behaviors of GH4169 Super Alloy and 3Cr2W8V Tool Steel Under Dry Rolling Condition [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(9): 983-996. | 
| [12] | Xiao-Pei Li, Song-Zhu Kure-Chu, Toru Ogasawara, Hitoshi Yashiro, Hai-Bo Wang, Zi-Zhen Xu, Xiao-Hui Li, Guo-Lin Song, Guo-Yi Tang. Fabrication of a Gradient Nano-/Micro-structured Surface Layer on an Al-Si Casting Alloy by Means of Ultrasonic-Electropulsing Coupling Rolling Process [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(12): 1258-1264. | 
| [13] | Yong-Da Ye, Xiao-Pei Li, Zhi-Yan Sun, Hai-Bo Wang, Guo-Yi Tang. Enhanced Surface Mechanical Properties and Microstructure Evolution of Commercial Pure Titanium Under Electropulsing-Assisted Ultrasonic Surface Rolling Process [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(12): 1272-1280. | 
| [14] | Ji-Ying Xia, Lin-Jiang Chai, Hao Wu, Yan Zhi, Yin-Ning Gou, Wei-Jiu Huang, Ning Guo. EBSD Study of Microstructural and Textural Changes of Hot-Rolled Ti-6Al-4V Sheet After Annealing at 800 °C [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(11): 1215-1223. | 
| [15] | M. Megahed, M. A. Attia, M. Abdelhameed, A. G. El-Shafei. Tribological Characterization of Hybrid Metal Matrix Composites Processed by Powder Metallurgy [J]. Acta Metallurgica Sinica (English Letters), 2017, 30(8): 781-790. | 
| Viewed | ||||||
| 
										Full text | 
									
										 | 
								|||||
| 
										Abstract | 
									
										 | 
								|||||
			   WeChat
			