Acta Metallurgica Sinica (English Letters) ›› 2015, Vol. 28 ›› Issue (2): 129-138.DOI: 10.1007/s40195-014-0172-x
• Orginal Article • Next Articles
Gang Liu1, Yu-Lai Xu1, Cai-Xiong Yang1, Xue-Shan Xiao1(), Xi-Min Chen2, Xiao-Ke Zhang2, Xiang-Jun Meng2
Received:
2014-05-16
Revised:
2014-07-07
Online:
2015-02-10
Published:
2015-07-23
Gang Liu, Yu-Lai Xu, Cai-Xiong Yang, Xue-Shan Xiao, Xi-Min Chen, Xiao-Ke Zhang, Xiang-Jun Meng. Effects of Alloy Elements on Oxidation Resistance and Stress-Rupture Property of P92 Steel[J]. Acta Metallurgica Sinica (English Letters), 2015, 28(2): 129-138.
Add to citation manager EndNote|Ris|BibTeX
Steel | C | N | Ce | Mn | Si | Cr | W | Mo | V | Nb | Ni | Ti | Fe |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
No. 1 | 0.095 | 0.054 | - | 0.42 | 0.26 | 8.73 | 1.83 | 0.51 | 0.21 | 0.06 | 0.30 | 0.01 | Bal. |
No. 2 | 0.103 | 0.049 | - | 0.42 | 0.28 | 9.38 | 1.97 | 0.48 | 0.21 | 0.06 | 0.29 | 0.01 | Bal. |
No. 3 | 0.093 | 0.054 | 0.02 | 0.42 | 0.26 | 8.72 | 1.83 | 0.51 | 0.19 | 0.06 | 0.30 | 0.01 | Bal. |
No. 4 | 0.093 | 0.052 | 0.02 | 0.41 | 0.78 | 8.71 | 1.83 | 0.50 | 0.21 | 0.06 | 0.30 | 0.01 | Bal. |
Table 1 Chemical compositions (wt%) of the steels
Steel | C | N | Ce | Mn | Si | Cr | W | Mo | V | Nb | Ni | Ti | Fe |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
No. 1 | 0.095 | 0.054 | - | 0.42 | 0.26 | 8.73 | 1.83 | 0.51 | 0.21 | 0.06 | 0.30 | 0.01 | Bal. |
No. 2 | 0.103 | 0.049 | - | 0.42 | 0.28 | 9.38 | 1.97 | 0.48 | 0.21 | 0.06 | 0.29 | 0.01 | Bal. |
No. 3 | 0.093 | 0.054 | 0.02 | 0.42 | 0.26 | 8.72 | 1.83 | 0.51 | 0.19 | 0.06 | 0.30 | 0.01 | Bal. |
No. 4 | 0.093 | 0.052 | 0.02 | 0.41 | 0.78 | 8.71 | 1.83 | 0.50 | 0.21 | 0.06 | 0.30 | 0.01 | Bal. |
Fig.3 The cross-section morphologies of No. 1 a, No. 2 b, No. 3 c, No. 4 d steels after oxidation at 750 °C for 700 h in air. The arrow in No. 1 shows the EDS line-scans direction. The areas spotted by laser beam in Raman analysis are marked by numbers
Species | Peak (cm-1) | |||||||||
---|---|---|---|---|---|---|---|---|---|---|
α-Fe2O3 | 226 | 245 | 296 | 411 | 495 | 612 | ||||
α-Fe2O3 | 225 | 245 | 295 | 415 | 500 | 615 | ||||
Fe3O4 | 550 | 670 | ||||||||
Fe3O4 | 300 | 320 | 420 | 560 | 680 | |||||
Cr2O3 | 303 | 351 | 397 | 530 | 550 | 609 |
Table 2 Locations (cm-1) of Raman-active vibrational modes of oxides of iron and chromium
Species | Peak (cm-1) | |||||||||
---|---|---|---|---|---|---|---|---|---|---|
α-Fe2O3 | 226 | 245 | 296 | 411 | 495 | 612 | ||||
α-Fe2O3 | 225 | 245 | 295 | 415 | 500 | 615 | ||||
Fe3O4 | 550 | 670 | ||||||||
Fe3O4 | 300 | 320 | 420 | 560 | 680 | |||||
Cr2O3 | 303 | 351 | 397 | 530 | 550 | 609 |
Fig.4 Raman spectra of the cross-section of No. 1 and No. 2 specimens corresponding to the regions in Fig. 3 a, b after oxidation at 750 °C for 700 h in air
Fig.5 Raman spectra of the cross-section of No. 3 and No. 4 specimens corresponding to the regions in Fig. 3 c, d after oxidation at 750 °C for 700 h in air
Fig. 6 EDS line-scans of cross-section of No. 1 steel after oxidation at 750 °C for 700 h in air with the scanning direction showing in Fig. 3a. The numbers correspond with those numbers in Fig. 3a
Fig. 7 Micrographs of No. 1 steel after heat treatment at 1,060 °C × 20 min AC + 765 °C × 3 h AC: a SEM micrograph, b The SEM-EDS of particles in Fig. 7 a; c, d, e TEM micrographs with diffraction patterns of M23C6 and Nb(C/N) particles
Fig. 8 TEM micrographs of No. 4 steel with diffraction patterns of Laves after heat treatment at 1,060 °C × 20 min AC + 765 °C × 3 h AC followed by aging at 625 °C × 1,000 h AC
Steel | Stress-Rupture life (h) | ε (%) | ψ (%) |
---|---|---|---|
No. 1 | 3,742 | 24 | 82 |
No. 2 | 4,523 | 24 | 83 |
No. 3 | 4,285 | 23 | 83 |
No. 4 | 2,021 | 22 | 80 |
Table 3 Variations of the stress-rupture life, elongation (ε) and reduction in area (ψ) with the test carried out first at 625 °C/125 MPa for 2,900 h and then at 625 °C/140 MPa to rupture (The stress-rupture life is the total time consumed by both parts of test)
Steel | Stress-Rupture life (h) | ε (%) | ψ (%) |
---|---|---|---|
No. 1 | 3,742 | 24 | 82 |
No. 2 | 4,523 | 24 | 83 |
No. 3 | 4,285 | 23 | 83 |
No. 4 | 2,021 | 22 | 80 |
Fig. 9 TEM micrographs of No. 1 a, No. 2 b, No. 3 c, No. 4 d steels after stress-rupture tests carried out first at 625 °C/125 MPa for 2,900 h and at 625 °C/140 MPa afterward
[1] | .F. Yin, W. Jung, S. Chung,Scripta Mater. 57, 469(2007) |
[2] | .X.Q. Hu, N.M. Xiao, X.H. Luo, D.Z. Li, J. Mater. Sci. Technol. 26, 817(2010) |
[3] | .L. Tan, X. Ren, T.R. Allen,Corros. Sci. 52, 1520(2010) |
[4] | .D. Laverde, T. Gόmez-Acebo, F. Castro,Corros. Sci. 46, 613(2004) |
[5] | .N.Q. Zhang, H. Xu, B.R. Li, Y. Bai, D.Y. Liu,Corros. Sci. 56, 123(2012) |
[6] | .A.S. Khanna, P. Rodriguez, J.B. Gnanamoorthy,Oxid. Met. 26, 171(1986) |
[7] | .I.G. Wright, B.A. Pint, Proceeding of NACE Corrosion 2002, Denver, CO, No. 02377(2002) |
[8] | .H.E. Evans, D.A. Hilton, R.A. Holm, S.J. Webster,Oxid. Met. 19, 1(1983) |
[9] | .Y. Suzuki, T. Yamashita, Y. Sugimoto, S. Fujita, S. Yamaguchi,ISIJ Int. 49, 564(2009) |
[10] | .T. Sundararajan, S. Kuroda, J. Kawakita, S. Seal, Surf. Coat. Technol. 201, 2124 (2006) |
[11] | .M. Schütze, M. Schorr, D.P. Renusch, A. Donchev, J.P.T. Vossen, J. Mater. Res. 7, 111(2004) |
[12] | .V. Lepingle, G. Louis, D. Allué, B. Lefebvre, B. Vandenberghe,Corros. Sci. 50, 1011(2008) |
[13] | .K.J. Yin, S.Y. Qiu, R. Tang, Q. Zhang, L.F. Zhang, J. Supercrit. Fluid. 50, 235(2009) |
[14] | .X.F. Wang, W.Q. Chen, J. Rare. Earths 28, 295 (2010) |
[15] | .N. Dudova, A. Plotnikova, D. Molodov, A. Belyakov, R. Kaibyshev, Mater. Sci. Eng. A 534, 632 (2012) |
[16] | .C.G. Panait, A. Zielińska-Lipiec, T. Koziel, A. Czyrska-Filemonowicz, A.F. Gourgues-Lorenzon, W. Bendick, Mater. Sci. Eng. A 527, 4062 (2010) |
[17] | .S.S. Wang, D.L. Peng, L. Chang, X.D. Hui,Mater. Des. 50, 174(2013) |
[18] | .P.J. Ennis, A. Zielinska-Lipiec, O. Wachter, A. Czyrska-Filemonowicz,Acta Mater. 45, 4901(1997) |
[19] | .R. Ma, Y.F. Yang, Q.Z. Yan, Y. Yang, X.G. Li, Acta Metall. Sin. (Engl. Lett.) 23, 451(2010) |
[20] | .P. Hu, W. Yan, W. Sha, W. Wang, Y.Y. Shan, K. Yang, J. Mater. Sci. Technol. 27, 344(2011) |
[21] | .C.S. Jeong, S.Y. Bae, D.H. Ki, K. Watanabe, B.S. Lim,Mater. Sci. Eng. A 449-451, 155(2007) |
[22] | .Q.M. Jin, J. Li, Y.L. Xu, X.S. Xiao,Corros. Sci. 52, 2846(2010) |
[23] | .Y.L. Xu, Q.M. Jin, J. Li, X.S. Xiao, X. Zhang, L.Z. Jiang,Corros. Sci. 52, 2846(2010) |
[24] | .F.H. Yu, G.H. Yang, R.D. Han, H.M. Weng,Acta Metall. Sin. 28, 49(1992). (in Chinese) |
[25] | .A.M. Huntz, V. Bague, G. Beauplé, C. Haut, C. Sévérac, P. Lecour, X. Longaygue, F. Ropital,Appl. Surf. Sci. 207, 255(2003) |
[26] | .G.H. Meier, K. Jung, N. Mu, N.M. Yanar, F.S. Pettit, J.P. Abellán, T. Olszewski, L.N. Hierro, W.J. Quadakkers, G.R. Holcomb,Oxid. Met. 74, 319(2010) |
[27] | .A. Kipelova, R. Kaibyshev, A. Belyakov, D. Molodov, Mater. Sci. Eng. A 528, 1280 (2011) |
[28] | .Z.X. Yuan, S.H. Song, T.H. Xi, X.J. Zhang, Z.S. Yu, Acta Metall. Sin. (Engl. Lett.) 10, 349(1997) |
[29] | .K. Laha, J. Kyono, T. Sasaki, S. Kishimoto, N. Shinya, Metall. Mater. Trans. A 36, 399 (2005) |
[30] | .Y.L. Xu, H. Nie, J. Li, X.S. Xiao, Mater. Sci. Eng. A 528, 643 (2010) |
[31] | .M.J. Cieslak, T.J. Headley, T. Kollie, A.D. Romig, Metall. Trans. A 19, 2319 (1988) |
[32] | .J.T. Guo, C. Shi,Acta Metall. Sin. 14, 348(1978). (in Chinese) |
[1] | Chun-Hua Ma, Fu-Sheng Pan, Ding-Fei Zhang, Ai-Tao Tang, Zhi-Wen Lu. Effects of Sb Addition on Microstructural Evolution and Mechanical Properties of Mg-9Al-5Sn Alloy [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(2): 278-288. |
[2] | L. B. Tong, J. H. Chu, D. N. Zou, Q. Sun, S. Kamado, H. G. Brokmeier, M. Y. Zheng. Simultaneously Enhanced Mechanical Properties and Damping Capacities of ZK60 Mg Alloys Processed by Multi-Directional Forging [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(2): 265-277. |
[3] | Meichen Liang, Hao Zhang, Lifeng Zhang, Peng Xue, Dingrui Ni, Weizhen Wang, Zongyi Ma, Hengqiang Ye, Zhiqing Yang. Evolution of Quasicrystals and Long-Period Stacking Ordered Structures During Severe Plastic Deformation and Mixing of Dissimilar Mg Alloys Upon Friction Stir Welding [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 12-24. |
[4] | Jinglin Liu, Qi Song, Lihui Song, Shude Ji, Mingshen Li, Zhen Jia, Kang Yang. A Novel Friction Stir Spot Riveting of Al/Cu Dissimilar Materials [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 135-144. |
[5] | Xudong Du, Feng Wang, Zhi Wang, Xingxing Li, Zheng Liu, Pingli Mao. Hot Tearing Susceptibility of AXJ530 Alloy Under Low-Frequency Alternating Magnetic Field [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1259-1270. |
[6] | Chao-Yue Zhao, Xian-Hua Chen, Peng Peng, Teng Tu, Andrej Atrens, Fu-Sheng Pan. Microstructures and Mechanical Properties of Mg-xAl-1Sn-0.3Mn (x = 1, 3, 5) Alloy Sheets [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1217-1225. |
[7] | Dan-Yang Liu, Jin-Feng Li, Yong-Cheng Lin, Peng-Cheng Ma, Yong-Lai Chen, Xu-Hu Zhang, Rui-Feng Zhang. Cu/Li Ratio on the Microstructure Evolution and Corrosion Behaviors of Al-xCu-yLi-Mg Alloys [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1201-1216. |
[8] | Yuan Yu, Peiying Shi, Kai Feng, Jiongjie Liu, Jun Cheng, Zhuhui Qiao, Jun Yang, Jinshan Li, Weimin Liu. Effects of Ti and Cu on the Microstructure Evolution of AlCoCrFeNi High-Entropy Alloy During Heat Treatment [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1077-1090. |
[9] | Hui Jiang, Tian-Dang Huang, Chao Su, Hong-Bin Zhang, Kai-Ming Han, Sheng-Xue Qin. Microstructure and Mechanical Behavior of CrFeNi2V0.5Wx (x = 0, 0.25) High-Entropy Alloys [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1117-1123. |
[10] | Ibrahim Ondicho, Bernard Alunda, Dicken Owino, Luke Otieno, Melody Chepkoech. Revealing a Transformation-Induced Plasticity (TRIP) Phenomenon in a Medium-Entropy Alloy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1159-1165. |
[11] | Qiuxin Nie, Hui Liang, Dongxu Qiao, Zhaoxin Qi, Zhiqiang Cao. Microstructures and Mechanical Properties of Multi-component AlxCrFe2Ni2Mo0.2 High-Entropy Alloys [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1135-1144. |
[12] | Chengbo Yang, Jing Zhang, Meng Li, Xuejian Liu. Soft-Magnetic High-Entropy AlCoFeMnNi Alloys with Dual-Phase Microstructures Induced by Annealing [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1124-1134. |
[13] | Ren Li, Jing Ren, Guo-Jia Zhang, Jun-Yang He, Yi-Ping Lu, Tong-Min Wang, Ting-Ju Li. Novel (CoFe2NiV0.5Mo0.2)100-xNbx Eutectic High-Entropy Alloys with Excellent Combination of Mechanical and Corrosion Properties [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1046-1056. |
[14] | Ning Li, Cun-Lei Jia, Zhi-Wei Wang, Li-Hui Wu, Ding-Rui Ni, Zheng-Kun Li, Hua-Meng Fu, Peng Xue, Bo-Lv Xiao, Zong-Yi Ma, Yi Shao, Yun-Long Chang. Achieving a High-Strength CoCrFeNiCu High-Entropy Alloy with an Ultrafine-Grained Structure via Friction Stir Processing [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(7): 947-956. |
[15] | Zhigang Zhang, Xiaotong Lu, Jianrong Xu, Hongjie Luo. Characterization and Tribological Properties of Graphene/Copper Composites Fabricated by Electroless Plating and Powder Metallurgy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(7): 903-912. |
Viewed | ||||||
Full text |
|
|||||
Abstract |
|
|||||