Acta Metallurgica Sinica (English Letters) ›› 2019, Vol. 32 ›› Issue (9): 1142-1150.DOI: 10.1007/s40195-019-00906-2
Special Issue: 2019年复合材料专辑
• Orginal Article • Previous Articles Next Articles
Xin-Yu Ren1, Hai-Shui Ren1, Yong-Wang Kang2, Hua-Ping Xiong1(), Chong Pei1, Bo Chen1, Yao-Yong Cheng1, A. I. Ustinov3
Received:
2018-10-17
Revised:
2019-03-20
Online:
2019-09-10
Published:
2019-08-06
Xin-Yu Ren, Hai-Shui Ren, Yong-Wang Kang, Hua-Ping Xiong, Chong Pei, Bo Chen, Yao-Yong Cheng, A. I. Ustinov. Solid-State Diffusion Bonding of NbSS/Nb5Si3 Composite Using Ni/Al and Ti/Al Nanolayers[J]. Acta Metallurgica Sinica (English Letters), 2019, 32(9): 1142-1150.
Add to citation manager EndNote|Ris|BibTeX
Microzone | Concentration (at.%) | Deduced phases | ||||||
---|---|---|---|---|---|---|---|---|
Nb | Ti | Si | Al | Cr | Hf | O | ||
1 | 42.58 | 14.33 | 41.90 | 1.19 | - | - | - | (Nb,Ti)5Si3 |
2 | 56.49 | 30.39 | - | 5.14 | 7.98 | - | - | (Nb,Ti)SS |
3 | 41.11 | 11.83 | 44.08 | 2.98 | - | (Nb,Ti)5Si3 | ||
4 | - | - | - | - | - | 31.92 | 68.08 | HfO2 |
Table 1 EDS analysis results for the microzones marked with 1, 2, 3 and 4 in Fig. 1a
Microzone | Concentration (at.%) | Deduced phases | ||||||
---|---|---|---|---|---|---|---|---|
Nb | Ti | Si | Al | Cr | Hf | O | ||
1 | 42.58 | 14.33 | 41.90 | 1.19 | - | - | - | (Nb,Ti)5Si3 |
2 | 56.49 | 30.39 | - | 5.14 | 7.98 | - | - | (Nb,Ti)SS |
3 | 41.11 | 11.83 | 44.08 | 2.98 | - | (Nb,Ti)5Si3 | ||
4 | - | - | - | - | - | 31.92 | 68.08 | HfO2 |
Fig. 4 Back-scattered electron image of NbSS/Nb5Si3 joint bonded with Ni/Al nanolayer a, and microstructure details at a high magnification of the selected area (rectangle in a) b
Microzone | Concentration (at.%) | Deduced phases | |||||||
---|---|---|---|---|---|---|---|---|---|
Nb | Ti | Ni | Si | Al | Cr | Hf | O | ||
1 | 4.66 | 23.78 | 42.66 | 1.96 | 26.94 | - | - | - | AlNi2Ti |
2 | 2.59 | 22.74 | 49.84 | - | 23.91 | - | 0.92 | - | AlNi2Ti |
3 | 27.13 | 6.46 | 32.51 | 4.14 | 25.88 | 3.38 | 0.50 | - | AlNb2?+?Ni3Al |
4 | 32.29 | 6.40 | 23.79 | 7.51 | 24.79 | 5.22 | - | - | AlNb2?+?Ni3Al |
5 | - | 6.08 | 45.17 | - | 48.75 | - | - | - | NiAl dissolved with Ti |
6 | - | - | 5.42 | - | - | - | 32.47 | 62.11 | HfO2 |
7 | 43.70 | 22.32 | 6.60 | 27.38 | - | - | - | - | (Nb,Ti)SS/Nb5Si3 dissolved with Ni |
8 | 54.78 | 12.03 | 7.94 | 25.25 | - | - | - | - | (Nb,Ti)SS/Nb5Si3 dissolved with Ni |
9 | 37.62 | 16.36 | 19.65 | 6.87 | 11.43 | 8.07 | - | - | Reaction products of Ni-Al and (Nb,Ti)-rich phase |
10 | 42.83 | 12.49 | 21.12 | 8.36 | 11.78 | 3.42 | - | - | Reaction products of Ni-Al and (Nb,Ti)-rich phase |
Table 2 EDS analysis results for the microzones in Fig. 4b
Microzone | Concentration (at.%) | Deduced phases | |||||||
---|---|---|---|---|---|---|---|---|---|
Nb | Ti | Ni | Si | Al | Cr | Hf | O | ||
1 | 4.66 | 23.78 | 42.66 | 1.96 | 26.94 | - | - | - | AlNi2Ti |
2 | 2.59 | 22.74 | 49.84 | - | 23.91 | - | 0.92 | - | AlNi2Ti |
3 | 27.13 | 6.46 | 32.51 | 4.14 | 25.88 | 3.38 | 0.50 | - | AlNb2?+?Ni3Al |
4 | 32.29 | 6.40 | 23.79 | 7.51 | 24.79 | 5.22 | - | - | AlNb2?+?Ni3Al |
5 | - | 6.08 | 45.17 | - | 48.75 | - | - | - | NiAl dissolved with Ti |
6 | - | - | 5.42 | - | - | - | 32.47 | 62.11 | HfO2 |
7 | 43.70 | 22.32 | 6.60 | 27.38 | - | - | - | - | (Nb,Ti)SS/Nb5Si3 dissolved with Ni |
8 | 54.78 | 12.03 | 7.94 | 25.25 | - | - | - | - | (Nb,Ti)SS/Nb5Si3 dissolved with Ni |
9 | 37.62 | 16.36 | 19.65 | 6.87 | 11.43 | 8.07 | - | - | Reaction products of Ni-Al and (Nb,Ti)-rich phase |
10 | 42.83 | 12.49 | 21.12 | 8.36 | 11.78 | 3.42 | - | - | Reaction products of Ni-Al and (Nb,Ti)-rich phase |
Microzone | Concentration (at.%) | Deduced phases | |||
---|---|---|---|---|---|
Nb | Ti | Si | Al | ||
1 | - | 50.60 | - | 49.40 | TiAl |
2 | 13.61 | 42.74 | - | 43.65 | (Ti,Nb)Al |
3 | 18.33 | 46.09 | - | 35.58 | (Ti,Nb)Al |
4 | 15.71 | 35.93 | - | 48.36 | (Ti,Nb)Al |
5 | 30.22 | 34.31 | - | 35.47 | (Ti,Nb)2Al |
6 | 31.43 | 30.53 | 4.52 | 33.52 | (Ti,Nb)2Al |
7 | 31.89 | 32.13 | - | 35.98 | (Ti,Nb)2Al |
8 | 47.35 | 12.51 | 37.86 | 2.28 | (Nb,Ti)5Si3 |
Table 3 EDS analysis results for the microzones in Fig. 7b
Microzone | Concentration (at.%) | Deduced phases | |||
---|---|---|---|---|---|
Nb | Ti | Si | Al | ||
1 | - | 50.60 | - | 49.40 | TiAl |
2 | 13.61 | 42.74 | - | 43.65 | (Ti,Nb)Al |
3 | 18.33 | 46.09 | - | 35.58 | (Ti,Nb)Al |
4 | 15.71 | 35.93 | - | 48.36 | (Ti,Nb)Al |
5 | 30.22 | 34.31 | - | 35.47 | (Ti,Nb)2Al |
6 | 31.43 | 30.53 | 4.52 | 33.52 | (Ti,Nb)2Al |
7 | 31.89 | 32.13 | - | 35.98 | (Ti,Nb)2Al |
8 | 47.35 | 12.51 | 37.86 | 2.28 | (Nb,Ti)5Si3 |
|
[1] | Jinglin Liu, Qi Song, Lihui Song, Shude Ji, Mingshen Li, Zhen Jia, Kang Yang. A Novel Friction Stir Spot Riveting of Al/Cu Dissimilar Materials [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 135-144. |
[2] | Fengqiang Xiao, Dongpo Wang, Wenbin Hu, Lei Cui, Zhiming Gao, Lanju Zhou. Effect of Interlayers on Microstructure and Properties of 2205/Q235B Duplex Stainless Steel Clad Plate [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(5): 679-692. |
[3] | Hong-Qiang Zhang, Hai-Lin Bai, Qiang Jia, Wei Guo, Lei Liu, Gui-Sheng Zou. High Electrical and Thermal Conductivity of Nano-Ag Paste for Power Electronic Applications [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(11): 1543-1555. |
[4] | Jinglin Liu, Shiyu Niu, Rong Ren, Shude Ji, Lei Wang, Zan Lv. Improving Joint Morphologies and Tensile Strength of Al/Mg Dissimilar Alloys Friction Stir Lap Welding by Changing Zn Interlayer Thickness [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(11): 1385-1395. |
[5] | Osama Saber, Haifa Alomair, Mohamed Abu-Abdeen, Abdullah Aljaafari. Fast Degradation of Green Pollutants Through Nanonets and Nanofibers of the Al-Doped Zinc Oxide [J]. Acta Metallurgica Sinica (English Letters), 2018, 31(5): 533-546. |
[6] | Zhang Xin, Shi Xiaohong, Wang Jie, Li Hejun, Li Kezhi, Ren Yancai. Effect of Bonding Temperature on the Microstructures and Strengths of C/C Composite/GH3044 Alloy Joints by Partial Transient Liquid-Phase (PTLP) Bonding with Multiple Interlayers [J]. Acta Metallurgica Sinica (English Letters), 2014, 27(4): 663-669. |
[7] | Zongan LUO, Guanglei WANG, Guangming XIE, Lipeng WANG, Kun ZHAO. Interfacial Microstructure and Properties of a Vacuum Hot Roll-bonded Titanium-Stainless Steel Clad Plate with a Niobium Interlayer [J]. Acta Metallurgica Sinica (English Letters), 2013, 26(6): 754-760. |
[8] | Yuhua LIU, Jiandong HU, Yaping ZHANG, Zuoxing GUO, Yue YANG. Effect of parameters on interface of the brazed ZrO2 ceramic and Ti-6Al-4V joint using Ti-based amorphous filler [J]. Acta Metallurgica Sinica (English Letters), 2012, 25(2): 89-94. |
[9] | W.B. Han, K.F. Zhang, B. Wang, D.Z. Wu. Superplasticity and Diffusion Bonding of IN718 Superalloy [J]. Acta Metallurgica Sinica (English Letters), 2007, 20(4): 307-312 . |
[10] | P. He; J. H. Zhang; J. C. Feng and Y. Y. Qian (National Key Laboratory of Advanced Welding Production Technology, HIT, Harbin 150001, China). DIFFUSION BONDING OF TiAl TO Ti AND TC4 ALLOY [J]. Acta Metallurgica Sinica (English Letters), 2000, 13(1): 162-167. |
[11] | WANG Chengguo. PENG Qifeng. LIU Junhai, SUN XitaiShandong Polytechnic University. Jinan, ChinaZHU Jing. CAI QigongCentral Iron and Steel Research Institute. Ministry of Metallurgical Industry. Beijing, China Manuscript received 14 April, 1994. TENSILE-SHEAR STRENGTH AND BREAKING MORPHOLOGY FOR VIBRATION DAMPING LAMINATED STEEL SHEET [J]. Acta Metallurgica Sinica (English Letters), 1994, 7(2): 114-118. |
[12] | HUANG Yan;MA Longxiang Northeast Universtity of Technology,Shenyang,China lecturer,Department of Metalforming,Northeast University of Technology,Shenyang 110006,China. DIFFUSION BONDING OF SUPERPLASTIC AI ALLOY LC4 [J]. Acta Metallurgica Sinica (English Letters), 1993, 6(8): 116-121. |
[13] | HUANC Yan CUI Jianzhong MA Longxiang Northeast University of Technology,Shenyang. INTERFACIAL ATOMIC-REACTION MODEL FOR DIFFUSION BONDING OF METALS [J]. Acta Metallurgica Sinica (English Letters), 1992, 5(10): 268-273. |
Viewed | ||||||
Full text |
|
|||||
Abstract |
|
|||||