Acta Metallurgica Sinica (English Letters) ›› 2017, Vol. 30 ›› Issue (3): 261-271.DOI: 10.1007/s40195-016-0500-4
Special Issue: 高温合金专辑(2016-2017); 2017-2018高温合金专辑
• Orginal Article • Previous Articles Next Articles
Shuang Gao1,Jie-Shan Hou1,Kai-Xin Dong1,Lan-Zhang Zhou1()
Received:
2016-07-10
Online:
2017-03-16
Published:
2017-05-16
Shuang Gao,Jie-Shan Hou,Kai-Xin Dong,Lan-Zhang Zhou. Influences of Cooling Rate After Solution Treatment on Microstructural Evolution and Mechanical Properties of Superalloy Rene 80[J]. Acta Metallurgica Sinica (English Letters), 2017, 30(3): 261-271.
Add to citation manager EndNote|Ris|BibTeX
C | Cr | Co | W | Mo | Al | Ti | B | Zr | Ni |
---|---|---|---|---|---|---|---|---|---|
0.15 | 13.98 | 9.62 | 4.17 | 4.02 | 2.87 | 4.8 | 0.013 | 0.061 | Bal. |
Table 1 Chemical composition of the alloy (wt%)
C | Cr | Co | W | Mo | Al | Ti | B | Zr | Ni |
---|---|---|---|---|---|---|---|---|---|
0.15 | 13.98 | 9.62 | 4.17 | 4.02 | 2.87 | 4.8 | 0.013 | 0.061 | Bal. |
Sample code | Solution | Aging |
---|---|---|
WC | 1200 °C/2 h/WC | 1095 °C/4 h/AC + 1080 °C/4 h/AC + 870 °C/12 h/AC |
AC | 1200 °C/2 h/AC | |
FC | 1200 °C/2 h/FC |
Table 2 Heat treatment schedule
Sample code | Solution | Aging |
---|---|---|
WC | 1200 °C/2 h/WC | 1095 °C/4 h/AC + 1080 °C/4 h/AC + 870 °C/12 h/AC |
AC | 1200 °C/2 h/AC | |
FC | 1200 °C/2 h/FC |
Fig. 1 Microstructures of the as-cast experimental alloy and EDS analysis: a OM image showing the dendritic microstructure; b SEM micrograph showing MC carbides morphology in as-cast microstructure; c morphology of γ′ precipitates; d SEM micrograph showing γ-γ′ eutectic in detail; e EDS spectrum of Ti-rich MC carbide
Fig. 2 Effects of the cooling methods after solution treatment on the microstructures: a-cmicrostructures of WC, AC and FC samples, respectively, d-f corresponding γ′ image of WC, AC and FC samples, respectively
Fig. 3 SEM micrographs of γ′ precipitates in three samples at different aging heat treatment stages: a-c at 1095 °C/4 h/AC; d-f at 1080 °C/4 h/AC; g-i at 870 °C/12 h/AC. Insetsin upper right show hyperfine tertiary γ′ particles in the matrix as marked by thearrows
Heat treatment stage | WC | AC | FC | |||
---|---|---|---|---|---|---|
d (nm) | Area fraction (%) | d (nm) | Area fraction (%) | d (nm) | Area fraction (%) | |
1 | 295 ± 24 | 15.7 | 290 ± 34 | 16.5 | 316 ± 54 | 14.7 |
2 | 345 ± 46 | 19.8 | 355 ± 51 | 17.8 | 372 ± 35 | 15.9 |
3 | 391 ± 36 | 24.7 | 402 ± 21 | 29.2 | 415 ± 24 | 26.5 |
Table 3 Statistical size and area fraction of secondary γ′ precipitates at different aging heat treatment stages
Heat treatment stage | WC | AC | FC | |||
---|---|---|---|---|---|---|
d (nm) | Area fraction (%) | d (nm) | Area fraction (%) | d (nm) | Area fraction (%) | |
1 | 295 ± 24 | 15.7 | 290 ± 34 | 16.5 | 316 ± 54 | 14.7 |
2 | 345 ± 46 | 19.8 | 355 ± 51 | 17.8 | 372 ± 35 | 15.9 |
3 | 391 ± 36 | 24.7 | 402 ± 21 | 29.2 | 415 ± 24 | 26.5 |
Fig. 4 SEM microstructures of the carbides and grain boundaries (marked by dotted lines) of AC sample in different heat treatment stages of a 1095 °C/4 h/AC, b 1080 °C/4 h/AC, cBS-SEM microstructure after aging of 870 °C/12 h/AC
MC | M6C | M23C6 | ||||
---|---|---|---|---|---|---|
wt% | at.% | wt% | at.% | wt% | at.% | |
Al | 0.7 | 1.7 | 1.9 | 6.2 | 0.9 | 2.1 |
Mo | 26.0 | 19.3 | 44.5 | 39.9 | 9.9 | 6.3 |
Ti | 42.7 | 63.5 | 4.2 | 7.5 | 2.5 | 3.2 |
Cr | 1.6 | 2.2 | 14.0 | 23.4 | 51.9 | 60.4 |
Co | 0.3 | 0.3 | 1.0 | 1.4 | 2.8 | 2.8 |
Ni | 2.2 | 2.7 | 5.7 | 8.3 | 21.1 | 21.7 |
W | 26.5 | 10.2 | 28.8 | 13.5 | 10.9 | 3.6 |
Table 4 EDS analysis of different carbides
MC | M6C | M23C6 | ||||
---|---|---|---|---|---|---|
wt% | at.% | wt% | at.% | wt% | at.% | |
Al | 0.7 | 1.7 | 1.9 | 6.2 | 0.9 | 2.1 |
Mo | 26.0 | 19.3 | 44.5 | 39.9 | 9.9 | 6.3 |
Ti | 42.7 | 63.5 | 4.2 | 7.5 | 2.5 | 3.2 |
Cr | 1.6 | 2.2 | 14.0 | 23.4 | 51.9 | 60.4 |
Co | 0.3 | 0.3 | 1.0 | 1.4 | 2.8 | 2.8 |
Ni | 2.2 | 2.7 | 5.7 | 8.3 | 21.1 | 21.7 |
W | 26.5 | 10.2 | 28.8 | 13.5 | 10.9 | 3.6 |
Fig. 5 TEM microstructures and SAED patterns of the carbides on grain boundaries of AC sample at 870 °C/12 h/AC aging: aM6C topography, M6C SAED pattern (inset in upper right corner) and MC SAED pattern (inset in lower left corner); bM23C6 topography andM23C6 SAED pattern (inset)
Fig. 6 SEM images: aγ′ coarsening on grain boundary and γ′ depleting on both sides of grain boundary after 870 °C/12 h/AC, b corresponding higher magnification image
Sample code | Tensile test at 25 °C | Tensile test at 870 °C | Hardness (HRC) | ||||||
---|---|---|---|---|---|---|---|---|---|
YS (MPa) | UTS (MPa) | El (%) | RA (%) | YS (MPa) | UTS (MPa) | El (%) | RA (%) | ||
WC | - | 520.5 | - | - | - | 337.5 | - | - | 41.39 |
AC | 938 | 1108 | 6.1 | 8.2 | 585 | 795 | 18.7 | 29 | 41.49 |
FC | 937.5 | 1092 | 6.3 | 8 | 545 | 692.5 | 21 | 32.25 | 41.51 |
Table 5 Results of mechanical tests for three kinds of samples
Sample code | Tensile test at 25 °C | Tensile test at 870 °C | Hardness (HRC) | ||||||
---|---|---|---|---|---|---|---|---|---|
YS (MPa) | UTS (MPa) | El (%) | RA (%) | YS (MPa) | UTS (MPa) | El (%) | RA (%) | ||
WC | - | 520.5 | - | - | - | 337.5 | - | - | 41.39 |
AC | 938 | 1108 | 6.1 | 8.2 | 585 | 795 | 18.7 | 29 | 41.49 |
FC | 937.5 | 1092 | 6.3 | 8 | 545 | 692.5 | 21 | 32.25 | 41.51 |
|
[1] | Xi Zhao, Fa-Fa Yan, Zhi-Min Zhang, Peng-Cheng Gao, Shu-Chang Li. Influence of Heat Treatment on Precipitation Behavior and Mechanical Properties of Extruded AZ80 Magnesium Alloy [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 54-64. |
[2] | Yuan Yu, Peiying Shi, Kai Feng, Jiongjie Liu, Jun Cheng, Zhuhui Qiao, Jun Yang, Jinshan Li, Weimin Liu. Effects of Ti and Cu on the Microstructure Evolution of AlCoCrFeNi High-Entropy Alloy During Heat Treatment [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1077-1090. |
[3] | Guang-Lei Wang, Dong-Qing Qi, Ji-De Liu, Jin-Lai Liu, Yi-Zhou Zhou, Xu-Dong Sun, Hai-Feng Zhang, Xiao-Feng Sun. Effect of Interactions Among Elements on Diffusion Process Associated with γ′ Coarsening in a Ni-Based Single-Crystal Superalloy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(7): 1013-1020. |
[4] | Hui Li, Wan Du, Yi Liu. Molecular Dynamics Study of Tension Process of Ni-Based Superalloy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(5): 741-750. |
[5] | Xian-Kai Fan, Fu-Quan Li, Lei Liu, Hai-Chao Cui, Feng-Gui Lu, Xin-Hua Tang. Evolution of γ′ Particles in Ni-Based Superalloy Weld Joint and Its Effect on Impact Toughness During Long-Term Thermal Exposure [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(4): 561-572. |
[6] | Wen-Chao Dong, Ming-Yue Wen, Hui-Yong Pang, Shan-Ping Lu. Effect of Post-weld Tempering on the Microstructure and Mechanical Properties in the Simulated HAZs of a High-Strength-High-Toughness Combination Marine Engineering Steel [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(3): 391-402. |
[7] | Guercio Giuseppe Del, Manuela Galati, Abdollah Saboori, Paolo Fino, Luca Iuliano. Microstructure and Mechanical Performance of Ti-6Al-4V Lattice Structures Manufactured via Electron Beam Melting (EBM): A Review [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(2): 183-203. |
[8] | Song-Wei Wang, Hong-Wu Song, Yan Chen, Shi-Hong Zhang, Hai-Hong Li. Evolution of Annealing Twins and Recrystallization Texture in Thin-Walled Copper Tube During Heat Treatment [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(12): 1618-1626. |
[9] | Wei Song, Xin-Guang Wang, Jin-Guo Li, Ye-Shun Huang, Jie Meng, Yan-Hong Yang, Jin-Lai Liu, Ji-De Liu, Yi-Zhou Zhou, Xiao-Feng Sun. Role of Ru on the Microstructural Evolution During Long-Term Aging of Ni-Based Single Crystal Superalloys [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(12): 1689-1698. |
[10] | Xin He, Jianbo Zhang, Yuanyi Peng, Jingan Li, Jian Ding, Chang Liu, Xingchuan Xia, Xueguang Chen, Yongchang Liu. Microstructure Evolution of Primary γ′ Phase in Ni3Al-Based Superalloy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(12): 1709-1726. |
[11] | Liang Yang, Jun Li, Defang Tu, Joel C. J. Strickland, Qiaodan Hu, Hongbiao Dong, Jianguo Li. Reduced Annealing Time and Enhanced Magnetocaloric Effect of La(Fe, Al)13 Alloy by La-nonstoichiometry and Si-doping [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(11): 1535-1542. |
[12] | Xiao Li, Bo Guan, Yun-Fei Jia, Yun-Chang Xin, Cheng-Cheng Zhang, Xian-Cheng Zhang, Shan-Tung Tu. Microstructural Evolution, Mechanical Properties and Thermal Stability of Gradient Structured Pure Nickel [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(8): 951-960. |
[13] | An-Wen Zhang, Yan Yang, Sha Zhang, Dong Zhang, Wei-Hong Zhang, Da-Wei Han, Feng Qi, Yuan-Guo Tan, Xin Xin, Wen-Ru Sun. Distribution of Phosphorus and Its Effects on Precipitation Behaviors and Tensile Properties of IN718C Cast Superalloy [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(7): 887-899. |
[14] | Pei-Lin Zhang, Yu-Hong Zhao, Ruo-Peng Lu, Zhi-Bing Ding, Hua Hou. Microalloying Effect of Sn on Phase Transformation During Heat Treatment in Mg-Y-Zn-Zr Alloys [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(5): 550-558. |
[15] | Xiang-Wei Li, Li Wang, Xin-Gang Liu, Yao Wang, Jia-Sheng Dong, Lang-Hong Lou. Effect of Aging Heat Treatment on the Microstructure and Creep Properties of the Cast Ni-Based Superalloy at Low Temperature [J]. Acta Metallurgica Sinica (English Letters), 2019, 32(5): 651-658. |
Viewed | ||||||
Full text |
|
|||||
Abstract |
|
|||||