Acta Metallurgica Sinica (English Letters) ›› 2014, Vol. 27 ›› Issue (5): 816-824.DOI: 10.1007/s40195-014-0143-2
• Orginal Article • Previous Articles Next Articles
Wang D., L. Xiao B., R. Ni D., Y. Ma Z.()
Received:
2014-08-14
Revised:
2014-08-20
Online:
2014-09-19
Published:
2014-11-13
Wang D., L. Xiao B., R. Ni D., Y. Ma Z.. Friction Stir Welding of Discontinuously Reinforced Aluminum Matrix Composites: A Review[J]. Acta Metallurgica Sinica (English Letters), 2014, 27(5): 816-824.
Add to citation manager EndNote|Ris|BibTeX
Materials | Rotation rate (r/min) | Welding speed (mm/min) | Tool material | Wearing of tool | Welding distance (mm) |
---|---|---|---|---|---|
15 vol% B4Cp/6061Al [ | 670 | 114 | H13 tool steel | Serious | 254 |
20 vol% Al2O3p/6061Al [ | 500-2,000 | 60 | Standard tool steel | Serious | 310 |
15 vol% SiCp/2009Al [ | 600 | 50 | H13 tool steel | Serious | - |
20 vol% SiCp/A359 [ | 1,000 | 180-540 | Standard tool steel | Serious | 610 |
15 vol% SiCp/A356 [ | 1,200 | 30 | D2 tool steel | - | 60 |
25 vol% SiCp/2,009Al [ | 800 | 120 | TiAlN-coated HSS-steel | - | - |
10 vol% Al2O3p/7005Al [ | 600 | 300 | Ferro-Titanit alloy | - | - |
30 vol% SiCp/AC4A Al [ | 1,500-2,000 | 25-150 | WC-Co hard alloy | Normal | 240 |
30 vol% SiCp/A359 [ | 1,000 | 76 | WC-Co hard alloy | Normal | 1320 |
Table 1 Tool wearing of friction stir welded aluminum matrix composites
Materials | Rotation rate (r/min) | Welding speed (mm/min) | Tool material | Wearing of tool | Welding distance (mm) |
---|---|---|---|---|---|
15 vol% B4Cp/6061Al [ | 670 | 114 | H13 tool steel | Serious | 254 |
20 vol% Al2O3p/6061Al [ | 500-2,000 | 60 | Standard tool steel | Serious | 310 |
15 vol% SiCp/2009Al [ | 600 | 50 | H13 tool steel | Serious | - |
20 vol% SiCp/A359 [ | 1,000 | 180-540 | Standard tool steel | Serious | 610 |
15 vol% SiCp/A356 [ | 1,200 | 30 | D2 tool steel | - | 60 |
25 vol% SiCp/2,009Al [ | 800 | 120 | TiAlN-coated HSS-steel | - | - |
10 vol% Al2O3p/7005Al [ | 600 | 300 | Ferro-Titanit alloy | - | - |
30 vol% SiCp/AC4A Al [ | 1,500-2,000 | 25-150 | WC-Co hard alloy | Normal | 240 |
30 vol% SiCp/A359 [ | 1,000 | 76 | WC-Co hard alloy | Normal | 1320 |
Fig. 3 Typical macrograph of 15 vol% SiCp/2009Al joints welded at a traverse speed of 50 mm/min and various rotation rates: a 400 r/min; b 600 r/min [23]
Fig. 5 Quantitative measurements of particle size distribution in 15 vol% SiCp/2009Al joint and BM: a as-FSW sample; b BM perpendicular to the rolling direction; c BM along the rolling direction [28]
Fig. 6 TEM micrographs and SAED patterns of 17 vol% SiCp/2009Al joint at 800 mm/min: a BM; b low-hardness zone of HAZ; c nugget zone; d SAED pattern of Al2Cu phase, region marked by white arrow in c; e SAED pattern of the Al matrix 〈100〉 projection, region marked by black arrow in c [13]
Materials | Plate thickness (mm) | Rotation rate (r/min) | Welding speed (mm/min) | BM condition | YS (MPa) | UTS (MPa) | El (%) | Joint eff. (%) |
---|---|---|---|---|---|---|---|---|
22 vol% Al2O3p/6061 [ | 4 | 880 | 260 | Cast | - | 217 | - | 99 |
10 vol% TiB2/Al [ | 6 | 2,000 | 30 | Cast | - | 223-282 | 3.4-6.7 | 79-99 |
15 vol% Mg2Si/Al [ | 6 | 1,120 | 125 | Cast | - | 115 | - | 100 |
10 wt% ZrB2/6061 [ | 6 | 1,150 | 50 | Cast | - | 240 | 1 | 95 |
20 wt% AlNp/6061 [ | 6 | 1,200 | 55 | Cast | - | 225 | - | 93 |
10 vol% SiCp/6061 [ | 6 | 1,100 | 45 | Cast | 126 | 206 | 6.8 | 74 |
10 vol% Al2O3p/7005 [ | 7 | 600 | 300 | Extruded + T6 | 263 | 299 | 1.2 | 82 |
10 vol% Al2O3p/7005 [ | 7 | 800 | 56 | T6 | 245 | 260 | 0.58 | 84 |
20 vol% Al2O3p/6061 [ | 7 | 800 | 56 | T6 | 280 | 329 | 1.3 | 87 |
20 vol% Al2O3p/6061 [ | 7 | - | Extruded + T6 | 234 | 251 | - | 70 | |
20 vol% Al2O3p/6061 [ | 7 | - | Extruded + T6 | 193 | 262 | 2.8 | 72 | |
6 vol% B4C/6063 [ | 4.5 | 1,500 | 600 | Extruded + T5 | 125 | 172 | 2.5 | 62 |
10.5 vol% B4C/6063 [ | 4.5 | 1,500 | 600 | Extruded +T5 | 125 | 176 | 2.5 | 62 |
25 vol% SiCp/2124 [ | 15 | 550 | 75 | Forged + T6 | 407 | 552 | 2.6 | 74.4 |
17 vol% SiCp/2009 [ | 3 | 1,000 | 50 | Rolled + T351 | 278 | 443 | 4.7 | 77 |
17 vol% SiCp/2009 [ | 3 | 1,000 | 800 | Rolled + T4 | 341 | 501 | 3.5 | 97 |
Table 2 Tensile properties of friction stir welded aluminum matrix composites
Materials | Plate thickness (mm) | Rotation rate (r/min) | Welding speed (mm/min) | BM condition | YS (MPa) | UTS (MPa) | El (%) | Joint eff. (%) |
---|---|---|---|---|---|---|---|---|
22 vol% Al2O3p/6061 [ | 4 | 880 | 260 | Cast | - | 217 | - | 99 |
10 vol% TiB2/Al [ | 6 | 2,000 | 30 | Cast | - | 223-282 | 3.4-6.7 | 79-99 |
15 vol% Mg2Si/Al [ | 6 | 1,120 | 125 | Cast | - | 115 | - | 100 |
10 wt% ZrB2/6061 [ | 6 | 1,150 | 50 | Cast | - | 240 | 1 | 95 |
20 wt% AlNp/6061 [ | 6 | 1,200 | 55 | Cast | - | 225 | - | 93 |
10 vol% SiCp/6061 [ | 6 | 1,100 | 45 | Cast | 126 | 206 | 6.8 | 74 |
10 vol% Al2O3p/7005 [ | 7 | 600 | 300 | Extruded + T6 | 263 | 299 | 1.2 | 82 |
10 vol% Al2O3p/7005 [ | 7 | 800 | 56 | T6 | 245 | 260 | 0.58 | 84 |
20 vol% Al2O3p/6061 [ | 7 | 800 | 56 | T6 | 280 | 329 | 1.3 | 87 |
20 vol% Al2O3p/6061 [ | 7 | - | Extruded + T6 | 234 | 251 | - | 70 | |
20 vol% Al2O3p/6061 [ | 7 | - | Extruded + T6 | 193 | 262 | 2.8 | 72 | |
6 vol% B4C/6063 [ | 4.5 | 1,500 | 600 | Extruded + T5 | 125 | 172 | 2.5 | 62 |
10.5 vol% B4C/6063 [ | 4.5 | 1,500 | 600 | Extruded +T5 | 125 | 176 | 2.5 | 62 |
25 vol% SiCp/2124 [ | 15 | 550 | 75 | Forged + T6 | 407 | 552 | 2.6 | 74.4 |
17 vol% SiCp/2009 [ | 3 | 1,000 | 50 | Rolled + T351 | 278 | 443 | 4.7 | 77 |
17 vol% SiCp/2009 [ | 3 | 1,000 | 800 | Rolled + T4 | 341 | 501 | 3.5 | 97 |
[1] | S.C. Tjong, Z.Y. Ma, Mater. Sci. Eng. R 29, 49 (2000) |
[2] | D. Storjohann, O.M. Barabash, S.S. Babu, S.A. David, P.S. Sklad, E.E. Bloom, Metall. Mater. Trans. A 36, 3237 (2005) |
[3] | X.H. Wang, J.T. Niu, S.K. Guan, L.J. Wang, D.F. Cheng, Mater. Sci. Eng. A 499, 106 (2009) |
[4] | J. Guo, P. Gougeon, F. Nadeau, X.G. Chen,Can. Metall. Q. 51, 277(2012) |
[5] | R.S. Mishra, Z.Y. Ma, Mater. Sci. Eng. R 50, 1 (2005) |
[6] | A.H. Feng, B.L. Xiao, Z.Y. Ma,Compos. Sci. Technol. 68, 2141(2008) |
[7] | A. Pirondi, L. Collini, Int. J. Fatigue 31, 111 (2009) |
[8] | F. Khodabakhshi, H.G. Yazdabadi, A.H. Kokabi, A. Simchi, Mater. Sci. Eng. A 585, 222 (2013) |
[9] | D. Wang, Q.Z. Wang, B.L. Xiao, D.R. Ni, Z.Y. Ma,Acta Metall. Sin. 50, 489(2014). (in Chinese) |
[10] | D. Wang, B.L. Xiao, Q.Z. Wang, Z.Y. Ma,Mater. Des. 47, 243(2013) |
[11] | D.R. Ni, D.L. Chen, D. Wang, B.L. Xiao, Z.Y. Ma,Mater. Des. 51, 199(2013) |
[12] | L. Ceschini, I. Boromei, G. Minak, A. Morri, F. Tarterini,Compos. Sci. Technol. 67, 605(2007) |
[13] | D. Wang, Q.Z. Wang, B.L. Xiao, Z.Y. Ma, Mater. Sci. Eng. A 589, 271 (2014) |
[14] | T. Prater, A. Strauss, G. Cook, B. Gibson, C. Cox, J. Mater. Eng. Perform. 22, 1807(2013) |
[15] | T.W. Nelson, H. Zhang, T. Haynes, in Proceedings of the Second Symposium on Friction Stir Welding, Gothenburg, Sweden, June 2000 |
[16] | R.A. Prado, L.E. Murr, D.J. Shindo, K.F. Sota,Scr. Mater. 45, 75(2001) |
[17] | A.H. Feng, Z.Y. Ma,Scr. Mater. 57, 1113(2007) |
[18] | D.J. Shindo, A.R. Rivera, L.E. Murr, J. Mater. Sci. 37, 4999(2002) |
[19] | M. Amirizad, A.H. Kokabi, M.A. Gharacheh, R. Sarrafi, B. Shalchi, M. Azizieh,Mater. Lett. 60, 565(2006) |
[20] | H. Uzun,Mater. Des. 28, 1440(2007) |
[21] | H.J. Liu, J.C. Feng, H. Fujiib, K. Nogi,Int. J. Mach. Tool Manu. 45, 1635(2005) |
[22] | R.A. Prado, L.E. Murr, K.F. Soto, J.C. Mc Clure, Mater. Sci. Eng. A 349, 156 (2003) |
[23] | Z.Y. Ma, A.H. Feng, B.L. Xiao, J.Z. Fan, L.K. Shi,Mater. Sci. Forum 539-543, 3814(2007) |
[24] | Y.N. Zhang, X. Cao, S. Larose, P. Wanjara,Can. Metall. Quart. 51, 250(2012) |
[25] | S.J. Vijay, N. Murugan,Mater. Des. 31, 3585(2010) |
[26] | P.A. Colegrove, H.R. Shercliff,Sci. Technol. Weld. Join. 9, 345(2004) |
[27] | W.M. Thomas, E.D. Nicholas, J.C. Needham, P. Temple-Smith, S.W.K.W. Kallee, C.J. Dawes, Friction stir welding, UK Patent, No. 2306366,(1996) |
[28] | L.M. Marzoli, A.V. Strombeck, J.F. Dos Santos, C. Gambaro, L.M. Volpone, Compos. Sci. Technol. 66, 363(2006) |
[29] | B. Inem, Mater. Sci. Eng., A 197, 91 (1995) |
[30] | X.X. Xia, H.J. Mcqueen,Appl. Compos. Mater. 4, 333(1997) |
[31] | D. Wang, Q.Z. Wang, B.L. Xiao, Z.Y. Ma, J. Mater. Sci. Technol. 30, 54(2014) |
[32] | Y.S. Sato, H. Kokawa, Metall. Mater. Trans. A 32, 3023 (2001) |
[33] | Z. Zhang, B.L. Xiao, Z.Y. Ma,Acta Mater. 73, 227(2014) |
[34] | R.D. Fu, J.F. Zhang, Y.J. Li, J. Kang, H.J. Liu, F.C. Zhang, Mater. Sci. Eng. A 559, 319 (2013) |
[35] | G. Minak, L. Ceschini, I. Boromei, M. Ponte, Int. J. Fatigue 32, 218 (2010) |
[36] | H. Nami, H. Adgi, M. Sharifitabar, H. Shamabadi,Mater. Des. 32, 976(2011) |
[37] | I. Dinaharana, N. Murugan, Mater. Sci. Eng. A 543, 257 (2012) |
[38] | N. Murugan, B. Ashok Kumar,Mater. Des. 51, 998(2013) |
[39] | P. Periyasamy, B. Mohan, V. Balasubramanian, J. Mater. Eng. Perform. 21, 2417(2012) |
[40] | P. Cavaliere, E. Cerri, L. Marzoli, J.D. Santos,Appl. Compos. Mater. 2, 247(2004) |
[41] | L. Ceschini, I. Boromei, G. Minak, A. Morri, F. Tarterini, Compos. Part A 38, 1200 (2007) |
[42] | X.G. Chen, M. da Silva, P. Gougeon, L. St-Georges, Mater. Sci. Eng. A 518, 174 (2009) |
[43] | F. Cioffi, R. Fernandez, D. Gesto, P. Rey, D. Verdera, G. Gonzalez-Doncel, Compos. Part A 54, 117 (2013) |
[44] | D.R. Ni, D.L. Chen, D. Wang, B.L. Xiao, Z.Y. Ma, Mater. Sci. Eng. A 608, 1 (2014) |
[45] | D.R. Ni, D.L. Chen, B.L. Xiao, D. Wang, Z.Y. Ma, Int. J. Fatigue 5, 64 (2013) |
[46] | A. Pirondi, L. Collini, D. Fersini,Eng. Fract. Mech. 75, 4333(2008) |
[1] | Chun-Hua Ma, Fu-Sheng Pan, Ding-Fei Zhang, Ai-Tao Tang, Zhi-Wen Lu. Effects of Sb Addition on Microstructural Evolution and Mechanical Properties of Mg-9Al-5Sn Alloy [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(2): 278-288. |
[2] | L. B. Tong, J. H. Chu, D. N. Zou, Q. Sun, S. Kamado, H. G. Brokmeier, M. Y. Zheng. Simultaneously Enhanced Mechanical Properties and Damping Capacities of ZK60 Mg Alloys Processed by Multi-Directional Forging [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(2): 265-277. |
[3] | S. Bi, B. L. Xiao, Z. H. Ji, B. S. Liu, Z. Y. Liu, Z. Y. Ma. Dispersion and Damage of Carbon Nanotubes in Carbon Nanotube/7055Al Composites During High-Energy Ball Milling Process [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(2): 196-204. |
[4] | Meichen Liang, Hao Zhang, Lifeng Zhang, Peng Xue, Dingrui Ni, Weizhen Wang, Zongyi Ma, Hengqiang Ye, Zhiqing Yang. Evolution of Quasicrystals and Long-Period Stacking Ordered Structures During Severe Plastic Deformation and Mixing of Dissimilar Mg Alloys Upon Friction Stir Welding [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 12-24. |
[5] | Jinglin Liu, Qi Song, Lihui Song, Shude Ji, Mingshen Li, Zhen Jia, Kang Yang. A Novel Friction Stir Spot Riveting of Al/Cu Dissimilar Materials [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 135-144. |
[6] | Quan Wen, Wenya Li, Vivek Patel, Luciano Bergmann, Benjamin Klusemann, Jorge F. dos Santos. Assessing the Bonding Interface Characteristics and Mechanical Properties of Bobbin Tool Friction Stir Welded Dissimilar Aluminum Alloy Joints [J]. Acta Metallurgica Sinica (English Letters), 2021, 34(1): 125-134. |
[7] | Dan-Yang Liu, Jin-Feng Li, Yong-Cheng Lin, Peng-Cheng Ma, Yong-Lai Chen, Xu-Hu Zhang, Rui-Feng Zhang. Cu/Li Ratio on the Microstructure Evolution and Corrosion Behaviors of Al-xCu-yLi-Mg Alloys [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1201-1216. |
[8] | Jing-Hua Liu, Jin-Jun Liu, Qiang Zheng, Bao-Ru Bian, Juan Du. In Situ Transmission Electron Microscopy Observations of the Growth Process of Fe3O4-Ag Nanoparticles [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1283-1288. |
[9] | Chao-Yue Zhao, Xian-Hua Chen, Peng Peng, Teng Tu, Andrej Atrens, Fu-Sheng Pan. Microstructures and Mechanical Properties of Mg-xAl-1Sn-0.3Mn (x = 1, 3, 5) Alloy Sheets [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1217-1225. |
[10] | Xudong Du, Feng Wang, Zhi Wang, Xingxing Li, Zheng Liu, Pingli Mao. Hot Tearing Susceptibility of AXJ530 Alloy Under Low-Frequency Alternating Magnetic Field [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1259-1270. |
[11] | Tianbo Zhao, Yutaka S. Sato, Hiroyuki Kokawa, Kazuhiro Ito. Predicting Tensile Properties of Friction-Stir-Welded 6063 Aluminum with Experimentally Measured Welding Heat Input [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(9): 1235-1242. |
[12] | Chengbo Yang, Jing Zhang, Meng Li, Xuejian Liu. Soft-Magnetic High-Entropy AlCoFeMnNi Alloys with Dual-Phase Microstructures Induced by Annealing [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1124-1134. |
[13] | Hao Wu, Si-Rui Huang, Cheng-Yan Zhu, Ji-Feng Zhang, He-Guo Zhu, Zong-Han Xie. In Situ TiC/FeCrNiCu High-Entropy Alloy Matrix Composites: Reaction Mechanism, Microstructure and Mechanical Properties [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1091-1102. |
[14] | Qiuxin Nie, Hui Liang, Dongxu Qiao, Zhaoxin Qi, Zhiqiang Cao. Microstructures and Mechanical Properties of Multi-component AlxCrFe2Ni2Mo0.2 High-Entropy Alloys [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1135-1144. |
[15] | Jinling Lu, Zhenjiang Wang, Wei Wang, Kexuan Zhou, Feng He, Zhijun Wang. Superior Slurry Erosion Behavior of a Casting NiCoCrFeNb0.45 Eutectic High Entropy Alloy [J]. Acta Metallurgica Sinica (English Letters), 2020, 33(8): 1111-1116. |
Viewed | ||||||
Full text |
|
|||||
Abstract |
|
|||||